Published: November 2026 |
By ZXD Engineering Team |
1. At what thickness does preheat become mandatory, and where is the upper limit?
Five conditions must hold at once before you can skip it: plate at or below 10–12 mm, CEV at or below about 0.45, low joint restraint, diffusible hydrogen at or below 5 mL/100 g, and a shop above 5 °C. That is what can you weld NM400 wear plate without preheating actually reduces to — a conjunction of five variables, not a yes/no property of the grade. Hydrogen cracking needs three things simultaneously: a hard martensitic HAZ, diffusible hydrogen, and tensile stress. Thickness controls cooling rate, CEV controls hardenability, restraint controls stress, and consumable handling controls hydrogen. Remove any one and the crack has no mechanism.
Use this NM400 wear plate preheat temperature by plate thickness chart as the WPS starting point. It is derived from CEV, thickness, heat input and hydrogen level under EN 1011-2 and ISO/TR 17671-2, not from the grade name:
|
Plate thickness |
Preheat at joint |
Heat input |
Interpass max |
Consumable |
Cooling |
|
6–10 mm |
20–80 °C; none if all five hold |
0.6–1.0 kJ/mm |
150 °C |
Basic low-hydrogen, 700–800 MPa |
Free air, dry |
|
10–20 mm |
80–120 °C |
0.8–1.2 kJ/mm |
200 °C |
Basic low-hydrogen or flux-cored |
Blanket on edge welds |
|
20–40 mm |
120–150 °C |
1.0–1.5 kJ/mm |
200–250 °C |
Low-hydrogen; austenitic for NM500 |
Blanket, slow cool below 100 °C |
|
Above 40 mm |
150–200 °C |
1.0–1.5 kJ/mm |
250 °C |
Austenitic or nickel-bearing |
Blanket, hold at least 4 h |
Mill data disagrees: some Chinese suppliers quote 120–180 °C for 10–20 mm NM400, Q&T plate guidance 80–120 °C. A NM400 wear plate preheat temperature by plate thickness chart only transfers between shops when CEV, hydrogen class and restraint match — ask for the mill certificate CEV before copying anyone's numbers.
Four things cancel the thin-plate exemption:
- Restraint. Box sections, gussets and T-joints raise tensile stress: add 20–30 °C, and weld transverse stiffeners before longitudinal seams.
- Cold shop. Below 5 °C, add 30–50 °C at every thickness and shield from wind.
- Hydrogen. Bake basic electrodes at 350–400 °C for one hour, keep them in a quiver, use within four hours. Above 10 mL/100 g, change consumable rather than extending the hold.
- Tack welds. Most field cracks start here: a tack is short, cools fastest, then gets locked in by the production weld. It needs the same preheat, cleaning and low-hydrogen treatment. Grind flame-cut faces back 1–2 mm.
Preheat a band at least 3t wide and never under 150–200 mm, and measure with a contact thermometer within 75 mm of the joint — the heater set point is not the plate temperature. Unequal thicknesses take the thicker member's value.
Jinhui Zhongxinde Machinery Parts (Tianjin) Co., Ltd. writes preheat as a range with both bounds, because a single minimum invites overshoot. ZXD records the measured value on the traveller for every NM400 and NM500 weld, so an OEM auditor can see the ceiling was respected.
✅ Bottom line: Below 10–12 mm preheat is optional only when CEV, restraint, hydrogen and shop temperature all cooperate; above 20 mm it is mandatory.

2. Why does the ceiling get tighter on NM500, and what does heat input do to it?
The upper limit is set by tempering response, not by cracking risk. NM500 is tempered in a lower range and carries less impact reserve, so time spent hot costs it more hardness. The interpass temperature for NM500 wear plate welding therefore has a tighter ceiling than NM400's. Preheat has two jobs — slowing cooling through the martensite range so the HAZ self-tempers, and drying moisture before the arc dissociates it into hydrogen. Neither improves above the tempering threshold; both start costing wear life.
The damage is quiet: published Q&T guidance puts the softened HAZ band at a 5–15 HRC drop, and a soak above roughly 200 °C softens the parent plate if the whole component is treated. A liner that passes every crack inspection can still wear through first in a 15–25 mm strip beside the weld. The 550–650 °C stress-relief rule belongs to carbon-steel vessels and plain structural frames; delete it from any wear-plate procedure.
Heat input is constrained both ways and is calculable: Q = 60 × V × I / (1000 × v) kJ/mm. At 24 V, 220 A and 250 mm/min that is about 1.27 kJ/mm. Too little means a hard HAZ above the ~350 HV cracking threshold; too much means a wide soft band and coarse grains.
- Stringer beads only, no wide weaving — narrow passes keep the soft band narrow.
- Undermatched, tough filler at 700–900 MPa for NM400, so the weld yields before the hard HAZ. Overmatching with high-carbon deposit adds risk without benefit.
- Austenitic or nickel-bearing consumables above NM500, which hold hydrogen in solution instead of releasing it into the HAZ.
- Grind the weld toes on cyclically loaded parts; the toe is both the notch and the hardest HAZ location.
- Slow cool under a blanket to below 100 °C on thick sections.
Treat the interpass temperature for NM500 wear plate welding as a hard stop measured on the plate: past 200–250 °C, stop and let it cool instead of continuing "while it is hot". Then bake out hydrogen at 200–250 °C for 2–4 hours (1–2 h at ≤5 mL/100 g, plus 0.5 h per extra 25 mm), ramp at ≤100 °C/h and cool to below 150 °C before air cooling. That hold is diffusion, not stress relief.
ZXD qualifies these ranges against the actual mill certificate on each OEM program; two plates both sold as 400 HBW can have different CEV and tempering response. We would rather quote a lower ceiling than deliver a part that is crack-free and worn out early.
✅ Bottom line: Preheat has a ceiling as well as a floor; beyond 200–250 °C you trade a crack for a soft band that wears through first.

FAQ
Q: Can you skip preheat on a 6 mm NM400 liner if the shop is warm?
A: Usually yes, and this is the case behind can you weld NM400 wear plate without preheating — thin plate, low CEV, an open fillet, low-hydrogen wire. But tacks need the same preheat and cleanliness, and a liner plug-welded into a closed box is no longer low-restraint. ZXD checks the joint detail first.
Q: What happens if we preheat to 300 °C "to be safe"?
A: You move the failure mode. Cracking risk falls, but the Q&T plate re-tempers, the HAZ softens by 5–15 HRC and the band beside the weld wears through first. Ask your supplier for the interpass ceiling, not only the minimum preheat.
Q: Can you supply a qualified WPS for our OEM approval?
A: Yes. ZXD issues the WPS with preheat floor, interpass ceiling, heat input range, consumable hydrogen class and the PQR behind it. The mill certificate CEV is attached to it.
CTA: Send the thickness and the restraint, get the window
Send the drawing with plate thickness, grade, joint type, and whether the part is boxed or gusseted. ZXD will return the preheat floor, the interpass ceiling, the heat input range and the hydrogen class — before the first tack weld is laid.
As a fabrication supplier since 2010, Jinhui Zhongxinde Machinery Parts (Tianjin) Co., Ltd. operates two plants totalling 13,000 m² and seven production lines under ISO 9001, ISO 14001 and ISO 45001, supplying welded structural parts to Sumitomo, Terex and Metso and shipping to Canada, the UK, Australia and Indonesia.
Email the drawing with annual volume and the mill certificate. We will tell you whether preheat can be skipped, and where the temperature must never go.
|
|
|
|